温馨提示:
1. 部分包含数学公式或PPT动画的文件,查看预览时可能会显示错乱或异常,文件下载后无此问题,请放心下载。
2. 本文档由用户上传,版权归属用户,汇文网负责整理代发布。如果您对本文档版权有争议请及时联系客服。
3. 下载前请仔细阅读文档内容,确认文档内容符合您的需求后进行下载,若出现内容与标题不符可向本站投诉处理。
4. 下载文档时可能由于网络波动等原因无法下载或下载错误,付费完成后未能成功下载的用户请联系客服处理。
网站客服:3074922707
TM_D_1815_
_00_2021
Designation:D181500(Reapproved 2021)Standard Test Method forWater Absorption(Static)of Vegetable Tanned Leather1This standard is issued under the fixed designation D1815;the number immediately following the designation indicates the year oforiginal adoption or,in the case of revision,the year of last revision.A number in parentheses indicates the year of last reapproval.Asuperscript epsilon()indicates an editorial change since the last revision or reapproval.This standard has been approved for use by agencies of the U.S.Department of Defense.1.Scope1.1 This test method covers the determination of the amountof water absorbed by leather at 23 6 2 C by immersion understatic conditions.It may be used on all types of leather,but isparticularly adapted to vegetable-tanned sole leather.This testmethod does not apply to wet blue.1.2 This standard does not purport to address all of thesafety concerns,if any,associated with its use.It is theresponsibility of the user of this standard to establish appro-priate safety,health,and environmental practices and deter-mine the applicability of regulatory limitations prior to use.1.3 This international standard was developed in accor-dance with internationally recognized principles on standard-ization established in the Decision on Principles for theDevelopment of International Standards,Guides and Recom-mendations issued by the World Trade Organization TechnicalBarriers to Trade(TBT)Committee.2.Referenced Documents2.1 ASTM Standards:2D1516 Test Method for Width of LeatherD1517 Terminology Relating to LeatherD1813 Test Method for Measuring Thickness of LeatherTest Specimens3.Terminology3.1 For definitions of leather terms used in this standardrefer to Terminology D1517.4.Summary of Test Method4.1 In this test method the amount of water absorbed by aleather specimen is measured at room temperature with allsurfaces exposed to water.5.Significance and Use5.1 This test method is currently used to determine compli-ance with specifications for water absorption of impregnatedsole leather.The significance of the test method is limited bythe static conditions employed,and the results do not reflect thewater absorption under the dynamic conditions of flexing.Theresult may be corrected,if required,for any water-solublematerial removed from the leather during the test.6.Apparatus6.1 Immersion Dish,glass or other noncorrosive material,having a flat bottom at least 3 by 5 in.(76 by 127 mm).6.2 Balance,sensitive to 0.01 g.6.3 Steel Scale or Tape,conforming to the requirements inSection 4 of Test Method D1516.6.4 Thickness Gauge,conforming to the requirements inSection 4 of Test Method D1813.6.5 Blotting Paper or Filter Paper.6.6 Drying Oven.6.7 Pieces of Glass Rod,for supporting and weighting thespecimen.6.8 Crystallizing Dish,borosilicate glass,50 mm tall,70mm in outside diameter.7.Test Specimen7.1 The test specimen shall be a rectangle of leatherapproximately 2 by 4 in.(51 by 102 mm).7.2 Unless otherwise specified in the detail specification,one specimen from each test unit of sample shall be tested.8.Procedure8.1 Determine the length,width,and thickness of thespecimen in accordance with Test Method D1516 and TestMethod D1813.Calculate its volume in cubic centimetres.8.2 Weigh the specimen to the nearest 0.01 g and record thismass as W1.8.3 Place the specimen in the immersion dish in a horizontalposition with the grain side up.Support it on glass rods orbeads and weighted with pieces of glass rod to keep it1This test method is under the jurisdiction of ASTM Committee D31 on Leatherand is the direct responsibility of Subcommittee D31.07 on Physical Properties.Thistest method was developed in cooperation with the American Leather ChemistsAssn.(Standard Method E30 1956).Current edition approved Sept.1,2021.Published October 2021.Originallyapproved in 1962.Last previous edition approved in 2015 as D1815 00(2015).DOI:10.1520/D1815-00R21.2For referenced ASTM standards,visit the ASTM website,www.astm.org,orcontact ASTM Customer Service at serviceastm.org.For Annual Book of ASTMStandards volume information,refer to the standards Document Summary page onthe ASTM website.Copyright ASTM International,100 Barr Harbor Drive,PO Box C700,West Conshohocken,PA 19428-2959.United StatesThis international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for theDevelopment of International Standards,Guides and Recommendations issued by the World Trade Organization Technical Barriers to Trade(TBT)Committee.1immersed.Carefully pour distilled water at 23 6 2 C into thedish until the specimen is fully immersed,using at least 10 g ofwater per gram of specimen.8.4 Leave the specimen immersed for a period of 30 min,2h,or 24 h,as required.8.5 At the end of the immersion period,remove the speci-men and blot the surface water with filter paper.Weigh thespecimen immediately to the nearest 0.01 g and record thismass as W2.8.6 If a