温馨提示:
1. 部分包含数学公式或PPT动画的文件,查看预览时可能会显示错乱或异常,文件下载后无此问题,请放心下载。
2. 本文档由用户上传,版权归属用户,汇文网负责整理代发布。如果您对本文档版权有争议请及时联系客服。
3. 下载前请仔细阅读文档内容,确认文档内容符合您的需求后进行下载,若出现内容与标题不符可向本站投诉处理。
4. 下载文档时可能由于网络波动等原因无法下载或下载错误,付费完成后未能成功下载的用户请联系客服处理。
网站客服:3074922707
TM_D_2028_
_D_2028M_
_15
Designation:D2028/D2028M15Standard Specification forCutback Asphalt(Rapid-Curing Type)1This standard is issued under the fixed designation D2028/D2028M;the number immediately following the designation indicates theyear of original adoption or,in the case of revision,the year of last revision.A number in parentheses indicates the year of lastreapproval.A superscript epsilon()indicates an editorial change since the last revision or reapproval.1.Scope1.1 This specification covers cutback petroleum asphalts ofthe rapid-curing type for use in the construction and treatmentof pavements.1.2 The values stated in either SI units or inch-pound unitsare to be regarded separately as standard.The values stated ineach system may not be exact equivalents;therefore,eachsystem shall be used independently of the other.Combiningvalues from the two systems may result in non-conformancewith the standard.2.Referenced Documents2.1 ASTM Standards:2D5 Test Method for Penetration of Bituminous MaterialsD95 Test Method for Water in Petroleum Products andBituminous Materials by DistillationD113 Test Method for Ductility of Bituminous MaterialsD140 Practice for Sampling Bituminous MaterialsD402 Test Method for Distillation of Cutback AsphaltD2042 Test Method for Solubility of Asphalt Materials inTrichloroethyleneD2170 Test Method for Kinematic Viscosity of Asphalts(Bitumens)D2171 Test Method for Viscosity of Asphalts by VacuumCapillary ViscometerD3143 Test Method for Flash Point of Cutback Asphalt withTag Open-Cup ApparatusD7553 Test Method for Solubility of Asphalt Materials inN-Propyl Bromide3.Properties3.1 The cutback asphalt shall not foam when heated toapplication temperature and shall conform to the requirementsprescribed in Table 1.4.Test Methods4.1 The material shall be sampled in accordance withPractice D140,and the properties enumerated in this specifi-cation shall be determined in accordance with the followingASTM methods:4.1.1 Flash Point(Tag Open-Cup)Test Method D3143.4.1.2 Viscosity,KinematicTest Method D2170.4.1.3 Viscosity,at 60C 140FTest Method D2171.4.1.4 DistillationTest Method D402.NOTE1If a 100-mL graduate does not permit sufficiently closereadings to determine conformity to these specifications with the desiredaccuracy,receivers graduated in 0.1-mL divisions shall be used.4.1.5 PenetrationTest Method D5.4.1.6 DuctilityTest Method D113.4.1.7 Solubility in Trichloroethylene or N-Propyl BromideTest Method D2042/D7553.4.1.8 WaterTest Method D95.1This specification is under the jurisdiction of ASTM Committee D04 on Roadand Paving Materials and is the direct responsibility of Subcommittee D04.40 onAsphalt Specifications.Current edition approved Jan.1,2015.Published January 2015.Originallyapproved in 1963.Last previous edition approved in 2010 as D2028/D2028M 10.DOI:10.1520/D2028_D2028M-15.2For referenced ASTM standards,visit the ASTM website,www.astm.org,orcontact ASTM Customer Service at serviceastm.org.For Annual Book of ASTMStandards volume information,refer to the standards Document Summary page onthe ASTM website.Copyright ASTM International,100 Barr Harbor Drive,PO Box C700,West Conshohocken,PA 19428-2959.United States1 ASTM International takes no position respecting the validity of any patent rights asserted in connection with any item mentionedin this standard.Users of this standard are expressly advised that determination of the validity of any such patent rights,and the riskof infringement of such rights,are entirely their own responsibility.This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years andif not revised,either reapproved or withdrawn.Your comments are invited either for revision of this standard or for additional standardsand should be addressed to ASTM International Headquarters.Your comments will receive careful consideration at a meeting of theresponsible technical committee,which you may attend.If you feel that your comments have not received a fair hearing you shouldmake your views known to the ASTM Committee on Standards,at the address shown below.This standard is copyrighted by ASTM International,100 Barr Harbor Drive,PO Box C700,West Conshohocken,PA 19428-2959,United States.Individual reprints(single or multiple copies)of this standard may be obtained by contacting ASTM at the aboveaddress or at 610-832-9585(phone),610-832-9555(fax),or serviceastm.org(e-mail);or through the ASTM website(www.astm.org).Permission rights to photocopy the standard may also be secured from the Copyright Clearance Center,222Rosewood Drive,Danvers,MA 01923,Tel:(978)646-2600;http:/ 1 Requirements for Cutback Asphalt(Rapid-Curing Type)NOTE1If the ductility at 25C 77F is less than 100,the material will be acceptable if its ductility at 15C 59F is more than 100.DesignationRC-70RC-250RC-800RC-3000MinMaxMinMaxMinMaxMinMaxKinematic viscosity at 60C 140F,mm2s70140250500800160030006000Flash point(Tag open-cup),C F.2780.2780.2780.Distillation test:Distilla