温馨提示:
1. 部分包含数学公式或PPT动画的文件,查看预览时可能会显示错乱或异常,文件下载后无此问题,请放心下载。
2. 本文档由用户上传,版权归属用户,汇文网负责整理代发布。如果您对本文档版权有争议请及时联系客服。
3. 下载前请仔细阅读文档内容,确认文档内容符合您的需求后进行下载,若出现内容与标题不符可向本站投诉处理。
4. 下载文档时可能由于网络波动等原因无法下载或下载错误,付费完成后未能成功下载的用户请联系客服处理。
网站客服:3074922707
TM_D_3872_
_05_2019
Designation:D387205(Reapproved 2019)Standard Test Method forFerrous Iron in Iron Oxides1This standard is issued under the fixed designation D3872;the number immediately following the designation indicates the year oforiginal adoption or,in the case of revision,the year of last revision.A number in parentheses indicates the year of last reapproval.Asuperscript epsilon()indicates an editorial change since the last revision or reapproval.1.Scope1.1 This test method covers the quantitative determinationof ferrous oxide(FeO)by oxidation of ferrous iron(Fe+)in anacid solution to the ferric state(Fe+)and titration withpotassium dichromate using diphenylamine as the indicator.1.2 This test method is applicable to synthetic black ironoxide,natural black iron oxide,magnetite or brown iron oxidewhere part of the iron content is present in the ferrous state(Note 1).It is applicable to iron oxides where the ferrous ironcontent ranges from 50 to 0.20%.NOTE1Natural iron oxides and magnetite may contain traces ofmetallic iron that will be combined with and analyzed as FeO.1.3 This standard does not purport to address the safetyconcerns if any,problems associated with its use.It is theresponsibility of the user of this standard to establish appro-priate safety,health,and environmental practices and deter-mine the applicability of regulatory limitations prior to use.1.4 This international standard was developed in accor-dance with internationally recognized principles on standard-ization established in the Decision on Principles for theDevelopment of International Standards,Guides and Recom-mendations issued by the World Trade Organization TechnicalBarriers to Trade(TBT)Committee.2.Referenced Documents2.1 ASTM Standards:2D280 Test Methods for Hygroscopic Moisture(and OtherMatter Volatile Under the Test Conditions)in PigmentsD1193 Specification for Reagent Water3.Significance and Use3.1 This test method may be used for production qualitycontrol or specification acceptance.4.Apparatus4.1 The digestion apparatus consists of a standard 500-mLErlenmeyer flask fitted with a two-hole rubber stopper andglass tubing,as shown in Fig.1,to provide for the introductionof the inert gas and vent for gas and digestion fumes.5.Reagents5.1 Purity of ReagentsReagent grade chemicals shall beused in all tests.Unless otherwise indicated,it is intended thatall reagents shall conform to the specifications of the Commit-tee on Analytical Reagents of the American Chemical Society,where such specifications are available.3Other grades may beused,provided it is first ascertained that the reagent is ofsufficiently high purity to permit its use without lessening theaccuracy of the determination.5.2 Purity of WaterUnless otherwise indicated,referencesto water shall be understood to mean Type II of SpecificationD1193.5.3 Diphenylamine IndicatorDissolve 1 g of diphenylam-ine in 100 mL of concentrated(H2SO4)(sp gr 1.84).5.4 Hydrochloric Acid(1+1)Dilute concentrated hydro-chloric acid(HCl,sp gr 1.19)with an equal volume of reagentwater.5.5 Iron Ore,Standard,Sibley No.27-f.45.6 Potassium Dichromate,Standard Solution(0.1 N)Dissolve 4.904 g of K2Cr2O7in water and dilute to 1 L.Standardize against National Institute of Standards and Tech-nology standard sample No.27f of Sibley iron ore.Calculatethe Fe factor in grams per millilitre for the solution as:Fe5 W/V1(1)1This test method is under the jurisdiction of ASTM Committee D01 on Paintand Related Coatings,Materials,and Applications and is the direct responsibility ofSubcommittee D01.31 on Pigment Specifications.Current edition approved May 1,2019.Published May 2019.Originallyapproved in 1979.Last previous edition approved in 2011 as D3872 05(2011).DOI:10.1520/D3872-05R19.2For referenced ASTM standards,visit the ASTM website,www.astm.org,orcontact ASTM Customer Service at serviceastm.org.For Annual Book of ASTMStandards volume information,refer to the standards Document Summary page onthe ASTM website.3Reagent Chemicals,American Chemical Society Specifications,AmericanChemical Society,Washington,DC.For suggestions on the testing of reagents notlisted by the American Chemical Society,see Analar Standards for LaboratoryChemicals,BDH Ltd.,Poole,Dorset,U.K.,and the United States Pharmacopeiaand National Formulary,U.S.Pharmacopeial Convention,Inc.(USPC),Rockville,MD.4May be secured from National Institute of Standards and Technology,Depart-ment of Commerce,Washington,DC 20234.Other recognized primary ironstandard may be substituted.Copyright ASTM International,100 Barr Harbor Drive,PO Box C700,West Conshohocken,PA 19428-2959.United StatesThis international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for theDevelopment of International Standards,Guides and Recommendations issued by the World Trade Organization Technical Barriers to Trade(TBT)Committee.1 where:W=weight of Fe in the standard iron ore(not the solution,as there i